Technical Data Sheet
Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Environmental Stress Cracking Resistance | | ASTM D1693 | 80.0 | hr |
Melt Mass-Flow Rate | | JIS K7210 | 7.0 | g/10 min |
| | 内部方法 | 18.0 | wt% |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Flexural Modulus | | ASTM D747 | 27.0 | Mpa |
Tensile Elongation | 断裂 | JIS K7113 | 750 | % |
Tensile Strength | 断裂 | JIS K7113 | 9.00 | Mpa |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
Vicat Softening Temperature | | JIS K7206 | 60.0 | °C |
Brittleness Temperature | | JIS K7216 | < -75.0 | °C |
Melting temperature | | JIS K7121 | 89.0 | °C |
Ring and Ball Softening Point | | | 146 | °C |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Shore Hardness | 邵氏 A | JIS K7215 | 91 | |
Shore Hardness | 邵氏 D | JIS K7215 | 36 | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.