Technical Data Sheet
Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Modeling Shrinkage | TD:2.00mm | ISO294-4 | 0.80 | % |
Modeling Shrinkage | MD:2.00mm | ISO294-4 | 0.80 | % |
Moisture Absorption | Saturation,23°C | ISO62 | 0.30 | % |
Moisture Absorption | Equilibrium,23°C,50%RH | ISO62 | 0.12 | % |
Melt Mass-Flow Rate | 330°C/2.16kg | ISO1133 | 31 | g/10min |
Melt Volume flow Rate | 330°C/2.16kg | ISO1133 | 30.0 | cm3/10min |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Flexural Modulus | 23°C | ISO178 | 2400 | Mpa |
Flexural Strength | 23°C | ISO178 | 105 | Mpa |
Nominal Tensile Strain at Break | 23°C | ISO527-2/50 | >50 | % |
Tensile Stress | Yield,23°C | ISO527-2/50 | 71.0 | Mpa |
Tensile Strain | Yield,23°C | ISO527-2/50 | 6.6 | % |
Tensile Modulus | 23°C | ISO527-2/1 | 2400 | Mpa |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
Deflection Temperature Under Load? | 0.45MPa,Unannealed | ISO75-2/B | 161 | °C |
Deflection Temperature Under Load? | 1.8MPa,Unannealed | ISO75-2/A | 148 | °C |
RTIElec | | UL746 | 140 | °C |
Evolution Calendar intelligent importer | | UL746 | 130 | °C |
RTIStr | | UL746 | 140 | °C |
Vicat Softening Temperature | | ISO306/B120 | 173 | °C |
Linear thermal expansion coefficient | MD:23to55°C | ISO11359-2 | 6.5E-05 | cm/cm/°C |
Linear thermal expansion coefficient | TD:23to55°C | ISO11359-2 | 6.5E-05 | cm/cm/°C |
Electrical performance | Test Condition | Test Method | Test Result | Unit |
---|
Dielectric Strength | 23°C,1.00mm | IEC60243-1 | 35 | KV/mm |
Relative Permittivity | 23°C,100Hz | IEC60250 | 3.00 | |
Relative Permittivity | 23°C,1MHz | IEC60250 | 2.90 | |
Comparative Tracking Index | SolutionA | IEC60112 | 250 | V |
Comparative Tracking Index | SolutionB | IEC60112 | 125 | V |
Dissipation Factor? | 23°C,100Hz | IEC60250 | 1E-03 | |
Dissipation Factor? | 23°C,1MHz | IEC60250 | 9E-03 | |
Surface Resistivity | | IEC60093 | 1E+16 | ohms |
Volume Resistivity | 23°C | IEC60093 | 1E+17 | ohms·cm |
Impact Properties | Test Condition | Test Method | Test Result | Unit |
---|
Charpy Unnotched Impact Strength | -30°C | ISO179/1eU | NoBreak | |
Charpy Unnotched Impact Strength | 23°C | ISO179/1eU | NoBreak | |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Ball Indentation Hardness | | ISO2039-1 | 124 | Mpa |
optical performance | Test Condition | Test Method | Test Result | Unit |
---|
Index of Refraction | | ISO489 | 1.576 | |
Transmittance | 1000µm | ISO13468-2 | 89.0 | % |
Flammability | Test Condition | Test Method | Test Result | Unit |
---|
UL flame retardant rating | 1.5mm | UL94 | HB | |
Glow Wire Flammability Index | | IEC60695-2-12 | 850 | °C |
Oxygen Index | | ISO4589-2 | 26 | % |
Supplementary information | Test Condition | Test Method | Test Result | Unit |
---|
ElectrolyticalCorrosion | 23°C | IEC60426 | A1 | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.