Technical Data Sheet
Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Melt Mass-Flow Rate | 190°C/2.16 kg | ASTM D1238 | 0.040 | g/10 min |
Environmental Stress Cracking Resistance | 25% Igepal, F50 | ASTM D1693B | > 1000 | hr |
Density | | ASTM D1505 | 0.956 | g/cm³ |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Flexural Modulus | | ASTM D747 | 932 | Mpa |
Tensile Elongation | Break | ASTM D638 | 820 | % |
Flexural Modulus | | ASTM D790 | 1180 | Mpa |
Tensile Strength | Yield | ASTM D638 | 29.4 | Mpa |
Tensile Strength | Break | ASTM D638 | 38.2 | Mpa |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
Vicat Softening Temperature | | ASTM D15253 | 125 | °C |
Peak Melting Temperature | | ASTM D3418 | 125 | °C |
Extrusion | Test Condition | Test Method | Test Result | Unit |
---|
Cylinder Zone 1 Temp | | | 180 到 200 | °C |
Die Temperature | | | 190 到 210 | °C |
Cylinder Zone 3 Temp | | | 180 到 200 | °C |
Cylinder Zone 5 Temp | | | 180 到 200 | °C |
Impact Properties | Test Condition | Test Method | Test Result | Unit |
---|
Notched Izod Impact Strength | | ASTM D256 | 290 | J/m |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Shore Hardness | Shore D | ASTM D2240 | 64 | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.