Technical Data Sheet
Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Melt Mass-Flow Rate | 224°C/1.2kg | ASTMD1238 | 40 | g/10min |
Modeling Shrinkage | MD | ASTMD955 | -0.20到0.50 | % |
Modeling Shrinkage | TD | ASTMD955 | 0.60到0.80 | % |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Taber Abrasion Resistance | 1000g,H-22Wheel | ASTMD1044 | 20.0 | mg |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
Linear thermal expansion coefficient | MD | ASTMD696 | 1.7E-04 | cm/cm/°C |
Glass Transition Temperature | | DSC | -40.0 | °C |
Vicat Softening Temperature | | ASTMD15253 | 85.0 | °C |
Elastomers Properties | Test Condition | Test Method | Test Result | Unit |
---|
Tensile Stress | 50%Strain,3.20mm | ASTMD412 | 4.10 | Mpa |
Tensile Stress | 100%Strain,3.20mm | ASTMD412 | 5.50 | Mpa |
Tensile Stress | 300%Strain,3.20mm | ASTMD412 | 11.7 | Mpa |
Tensile Strength | Break,3.20mm | ASTMD412 | 34.5 | Mpa |
Tensile Elongation | Break,3.20mm | ASTMD412 | 600 | % |
Tearing Strength | 3.20mm | ASTMD624 | 105 | kN/m |
Compression Set | 25°C,22hr | ASTMD395B | 30 | % |
Compression Set | 70°C,22hr | ASTMD395B | 33 | % |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Shore Hardness | Shore A | ASTMD2240 | 82 | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.