Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Modeling Shrinkage | MD:3.20mm | 内部方法 | 0.80到1.0 | % |
Melt Mass-Flow Rate | 300°C/1.2kg | ASTMD1238 | 2.0 | g/10min |
Melt Volume flow Rate | 300°C/1.2kg | ISO1133 | 2.00 | cm3/10min |
Specific Volume | | ASTMD792 | 0.835 | cm³/g |
-- | | ASTMD792,ISO1183 | 1.20 | g/cm³ |
-- | | ASTMD792 | 1.19 | g/cm³ |
24hr | | ASTMD570 | 0.19 | % |
Saturation ,23℃ | | ISO62 | 0.16 | % |
Equilibrium,23°C,50%RH | | ISO62 | 0.35 | % |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
50.0mm Span | | ASTMD790 | 2330 | Mpa |
--7 | | ISO178 | 2070 | Mpa |
--8 | | ISO178 | 66.0 | Mpa |
--1 | | ASTMD638 | 2080 | Mpa |
Yield | | ASTMD638 | 8.0 | % |
Break | | ASTMD638 | 78 | % |
Yield,50.0mm Span | | ASTMD790 | 97.2 | Mpa |
yield | | ISO527-2/50 | 68.0 | Mpa |
yield | | ISO527-2/50 | 7.0 | % |
fracture | | ISO527-2/50 | 68.0 | Mpa |
fracture | | ISO527-2/50 | 100 | % |
Yield | | ASTMD638 | 65.5 | Mpa |
Break | | ASTMD638 | 77.9 | Mpa |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
1.8MPa, Unannealed,3.20mm | | ASTMD648 | 149 | °C |
Specific Heat | | ASTMC351 | 1260 | J/kg/°C |
Thermal Conductivity | | ASTMC177 | 0.21 | W/m/K |
RTIElec | | UL746 | 130 | °C |
Evolution Calendar intelligent importer | | UL746 | 130 | °C |
-- | | ASTMD152514 | 173 | °C |
-- | | ISO306/B50 | 165 | °C |
-- | | ISO306/B120 | 167 | °C |
Flow:-40 to 40°C | | ASTME831,ISO11359-2 | 6E-05 | cm/cm/°C |
Flow:-40 to 40°C | | ASTME831,ISO11359-2 | 6E-05 | cm/cm/°C |
RTI | | UL746 | 130 | °C |
Flow:-40 to 95°C | | ASTME831 | 8.1E-05 | cm/cm/°C |
1.8MPa, Unannealed,64.0mm Span | | ISO75-2/Af | 150 | °C |
Electrical performance | Test Condition | Test Method | Test Result | Unit |
---|
Arc Resistance | | ASTMD495 | PLC6 | |
Dissipation Factor? | 50Hz | ASTMD150 | 1.6E-03 | |
Dissipation Factor? | 60Hz | ASTMD150 | 1.6E-03 | |
Dissipation Factor? | 100Hz | ASTMD150 | 0.026 | |
Dielectric Strength | 3.20mm,inAir | ASTMD149 | 20 | KV/mm |
Comparative Tracking Index | CTI | UL746 | PLC3 | |
Dielectric Constant | 50Hz | ASTMD150 | 3.27 | |
Dielectric Constant | 60Hz | ASTMD150 | 3.27 | |
Dielectric Constant | 1MHz | ASTMD150 | 3.10 | |
Volume Resistivity | | ASTMD257 | >2.5E+17 | ohms·cm |
Hot-wire Ignition | HWI | UL746 | PLC2 | |
High Amp Arc Ignition | HAI | UL746 | PLC3 | |
High Voltage Arc Tracking Rate | HVTR | UL746 | PLC3 | |
Impact Properties | Test Condition | Test Method | Test Result | Unit |
---|
Gardner Impact | 23°C | ASTMD3029 | 149 | J |
Instrumented Dart Impact | 23°C,TotalEnergy | ASTMD3763 | 74.0 | J |
Unnotched Izod Impact Strength | 23°C | ASTMD4812 | 3200 | J/m |
-30°C | | ASTMD256 | 84 | J/m |
23°C | | ASTMD256 | 370 | J/m |
Tensile Impact Strength | | ASTMD1822 | 578 | kJ/m² |
-30°C10 | | ISO180/1A | 6.0 | kJ/m² |
23°C11 | | ISO180/1A | 7.0 | kJ/m² |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Rockwell Hardness | M-Scale | ASTMD785 | 92 | |
Rockwell Hardness | R-Scale | ASTMD785 | 127 | |
optical performance | Test Condition | Test Method | Test Result | Unit |
---|
Transmittance | 2540µm | ASTMD1003 | 85.0 | % |
Refractive index of light | | ASTMD542 | 1.600 | |
Haze | 2540µm | ASTMD1003 | 1.0 | % |
Flammability | Test Condition | Test Method | Test Result | Unit |
---|
UL flame retardant rating | 1.47mm | UL94 | HB | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.