Technical Data Sheet
Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Modeling Shrinkage | MD | 内部方法 | 1.5到2.5 | % |
Moisture Absorption | Equilibrium | ASTMD570 | <0.010 | % |
Melt Mass-Flow Rate | 190°C/2.16kg | ASTMD1238 | 0.035 | g/10min |
Density / Specific Gravity | | ASTMD1505 | 0.957 | g/cm³ |
Environmental Stress Cracking Resistance | | ASTMD1693B | >1000 | hr |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Tensile Elongation | Break | ASTMD638 | >500 | % |
Flexural Modulus | | ASTMD790 | 981 | Mpa |
Tensile Strength | Yield | ASTMD638 | 39.2 | Mpa |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
Vicat Softening Temperature | | ASTMD1525 | 123 | °C |
Deflection Temperature Under Load? | 1.8MPa,Unannealed | ASTMD648 | 62.0 | °C |
Peak Melting Temperature | | ASTMD3418 | 134 | °C |
Brittleness Temperature | | ASTMD746 | <-70.0 | °C |
Impact Properties | Test Condition | Test Method | Test Result | Unit |
---|
Notched Izod Impact Strength | | ASTMD256 | >490 | J/m |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Rockwell Hardness | R-Scale | ASTMD785 | 47 | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.