Technical Data Sheet
Physical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Modeling Shrinkage | MD:--2 | 内部方法 | 0.50to0.80 | % |
Modeling Shrinkage | MD:--3 | 内部方法 | 0.30to0.50 | % |
Modeling Shrinkage | TD:--3 | 内部方法 | 0.40to0.60 | % |
Modeling Shrinkage | TD:--4 | 内部方法 | 0.60to0.90 | % |
Moisture Absorption | 24hr | ASTMD570 | 0.070 | % |
Specific Volume | | ASTMD792 | 0.640 | cm³/g |
Outdoor Suitability | | UL746C | f1 | |
Density / Specific Gravity | | ASTMD792 | 1.59 | g/cm³ |
Mechanical Properties | Test Condition | Test Method | Test Result | Unit |
---|
Flexural Modulus | 50.0mmSpan | ASTMD790 | 9400 | Mpa |
Flexural Strength | Break,50.0mmSpan | ASTMD790 | 179 | Mpa |
Tensile Strength | Break | ASTMD638 | 110 | Mpa |
Thermal Properties | Test Condition | Test Method | Test Result | Unit |
---|
Deflection Temperature Under Load? | 0.45MPa,Unannealed,6.40mm | ASTMD648 | 204 | °C |
Deflection Temperature Under Load? | 1.8MPa,Unannealed,6.40mm | ASTMD648 | 160 | °C |
RTIElec | | UL746 | 125 | °C |
Evolution Calendar intelligent importer | | UL746 | 110 | °C |
RTIStr | | UL746 | 125 | °C |
Linear thermal expansion coefficient | MD:-40to40°C | ASTME831 | 2.2E-05 | cm/cm/°C |
Linear thermal expansion coefficient | MD:60to138°C | ASTME831 | 2.2E-05 | cm/cm/°C |
Electrical performance | Test Condition | Test Method | Test Result | Unit |
---|
Dielectric Strength | 1.60mm,in Oil | ASTMD149 | 26 | KV/mm |
Dielectric Strength | 3.20mm,inAir | ASTMD149 | 19 | KV/mm |
Comparative Tracking Index | CTI | UL746 | PLC3 | |
Arc Resistance | | ASTMD495 | PLC6 | |
Dissipation Factor? | 100Hz | ASTMD150 | 2E-03 | |
Dissipation Factor? | 1MHz | ASTMD150 | 0.020 | |
Dielectric Constant | 100Hz | ASTMD150 | 3.80 | |
Dielectric Constant | 1MHz | ASTMD150 | 3.70 | |
Volume Resistivity | | ASTMD257 | 4.3E+16 | ohms·cm |
Hot-wire Ignition | HWI | UL746 | PLC1 | |
High Amp Arc Ignition | HAI | UL746 | PLC3 | |
High Voltage Arc Tracking Rate | HVTR | UL746 | PLC3 | |
Impact Properties | Test Condition | Test Method | Test Result | Unit |
---|
Notched Izod Impact Strength | 23°C | ASTMD4812 | 640 | J/m |
Notched Izod Impact Strength | 23°C | ASTMD256 | 85 | J/m |
hardness | Test Condition | Test Method | Test Result | Unit |
---|
Rockwell Hardness | R-Scale | ASTMD785 | 118 | |
Flammability | Test Condition | Test Method | Test Result | Unit |
---|
Oxygen Index | | ASTMD2863 | 37 | % |
UL flame retardant rating | 0.9mm | UL94 | V-0 | |
UL flame retardant rating | 2.3mm | UL94 | 5VA | |
IMPORTANT NOTES: Plas.com collected the data in the data sheet from the material manufacturers. Plas.com makes the best effort to improve the accuracy of the data, but has no responsibility for the data. We strongly recommend verifying the validity of the data with the material manufacturers before making a final decision.